http://chineseinput.net/에서 pinyin(병음)방식으로 중국어를 변환할 수 있습니다.
변환된 중국어를 복사하여 사용하시면 됩니다.
Development of Tungsten Dispersed Copper Based Alloy and its Physical Property
Mishima, Akira,Sakaguchi, Shigeya Korean Powder Metallurgy Institute 1998 한국분말재료학회지 (KPMI) Vol.5 No.4
Copper-10 wt. % tungsten alloyed powder was obtained by co-reduction of mixed tungsten-trioxide and copper oxide powders at 973 K for 7.2 Ks. In the alloy obtained by pressure-assisted sintering of this co-reduced powder, ultra fine tungsten particles (about 100nm) were dispersed uniformly in the copper matrix. At room temperature, the hardness of this alloy was Hv151 and the electrical conductivity was 85% IACS. After annealing at 1173 K for 3.6 Ks, the hardness and electrical conductivity were Hv147 and 84% IACS, respectively, and were same as before annealing. It was confirmed that the hardness and electrical conductivity of this alloy were hardly influenced by annealing condition since the microstructure of this alloy is highly stabilized.