http://chineseinput.net/에서 pinyin(병음)방식으로 중국어를 변환할 수 있습니다.
변환된 중국어를 복사하여 사용하시면 됩니다.
펄스 전류 하에서 AZ31 마그네슘 합금의 플라즈마전해산화 피막의 형성 거동
문성모 한국표면공학회 2022 한국표면공학회지 Vol.55 No.5
In this study, PEO (plasma electrolytic oxidation) film formation behavior of AZ31 Mg alloy under application of 300 Hz pulse current was studied by the analyses of V-t curve, arc generation behavior, PEO film thickness and morphology of PEO films with treatment time in 0.05 M NaOH + 0.05 M Na2SiO3 + 0.1 M NaF solution. PEO films was observed to grow after 10 s of application of pulse current together with generation of micro-arcs. PEO film grew linearly with treatment time at a growth rate of about 5.58 ㎛/min at 200 mA/cm2 of pulse current but increasing rate of film formation voltage became lowered largely with increasing treatment time after passing about 250 V, suggesting that resistivity of PEO films during micro-arc generation decreases with increasing film formation voltage at more than 250 V.